Aesthetic ceramic coating applied over a baked resistant substructure based on ultra hard zircon and sodium oxide.
The mass gives the effect characteristic of natural teeth, transparent.
Dentin, Enamel, Clear, Neutral, Translucent, Modifier, Chroma, Mamelon, Gingiva
Coefficient of thermal expansion |
2 firing: 9.0 x 10-6 x K-1; 4 firing: 9,0 x 10-6 x K-1 |
Conversion temperature |
500°C ±10 |
Stain Powder Dye
Coefficient of thermal expansion |
9,8 x 10-6 x K-1; |
Conversion temperature |
510°C ±10 |
Opal Opal
Coefficient of thermal expansion |
2 firing: 12.5 – 13.5 x 10-6 x K-1; 4 firing: 12,5 – 13,5 x 10-6 x K-1 |
Conversion temperature |
500°C ±10 |
| ZR (zirconium ceramics) | t° preheating | Drying time | t° of the beginning of the vacuum mode | Warm-up rate | Firing | Exposure time |
|---|---|---|---|---|---|---|
| Cleaning roasting | 500° C | 3 min. | 500° C | 65° C / min. | 980° C | 5 min. |
| 1st firing
Dentin / Enamel |
450° C | 6 min. | 450° C | 45° C / min. | 810° C | 1 min. |
| 2nd firing
Dentin / Enamel |
450° C | 6 min. | 450° C | 45° C / min. | 810° C | 1 min. |
| Glaze | 450° C | 3 min. | – | 45° C / min. | 800° C | 1 min. |